Tempered Glass

Tempered glass — also called toughened glass — is standard float glass that has been subjected to a controlled thermal tempering process. The result is a pane that is approximately four times stronger than annealed (ordinary) glass of the same thickness, and that breaks safely into small, blunt-edged fragments rather than large, sharp shards.

Applications and fabrication

It is the most widely specified safety glass in construction, required by building codes for applications such as entrance doors, sidelites, shower enclosures, glass railings, and any glazing within 18 inches of the floor.

Tempered vs. Laminated Glass

Tempered glass

Heat treatment increases the strength of the glass. When fully tempered glass breaks, it typically crumbles into many small fragments. Common applications include shower enclosures, glass doors and interior partitions.

Laminated glass

An interlayer bonds two or more panes and helps hold the fragments together if the glass breaks. This makes laminated glass a common option where fragment retention matters, such as overhead glazing or some railing systems.

Glass can be both tempered and laminated. For a specific installation, confirm the required glass construction, thickness, supports and applicable glazing requirements.

See how CAN-BEST tested the tempered specimens

Tempered Glass Safety Testing

Rez Glass Industries manufactures custom architectural glass for contractors and glaziers across the Greater Toronto Area. In report L24-1636-7070, issued June 19, 2024, CAN-BEST confirmed that our 6, 10 and 12 mm clear, fully tempered glass specimens passed Class A impact testing under CAN/CGSB-12.1-2022 and ANSI Z97.1-2015 (R2020). The lab evaluated four specimens per thickness. Each measured 864 × 1,930 mm (approximately 34 × 76 in.).

Class A impact test

The lab dropped a 100 lb (45.4 kg) impactor from 48 in. (1,220 mm) to strike near the centre of each panel. All 12 specimens remained intact.

Centre-punch fragmentation test

The lab then broke each specimen with a centre punch and weighed its ten largest fragments together. For every specimen, that weight was below the limit based on glass thickness.

Results by nominal thickness

  • 6 mm: all four specimens stayed intact after impact and passed fragmentation.
  • 10 mm: all four specimens stayed intact after impact and passed fragmentation.
  • 12 mm: all four specimens stayed intact after impact and passed fragmentation.

These results apply to the specimens tested. For project specifications, confirm the required glazing type, panel dimensions, and installation details for the intended application.

CAN-BEST Tempered Glass Safety Test Report L24-1636-7070 (PDF)